1.Qiymatlar, agar boshqacha ko'rsatilmagan bo'lsa, xona haroratida toroidal yadro P25×P15×10 bilan olingan.
2.Odatiy qiymat,*1Sinov sharti (f=400kHz,B=50mT),*2Test holati (f=500kHz,B=50mT).

product-833-482

 

Olchamlari (mm)

Asosiy parametrlar

A

80.0+2.0/-1.0

C1

0.485 mm-1

B

65.0±0.5

Le

314 mm

C

30.0±0.5

Ae

647 mm2

D

21.5±0.5

Ve

203000 mm3

E

37.0(Ref)

Massa

≈1010 g/prs

F

43.0±1.0

   

 

ELEKTR XUSUSIYATLARI

 

Elementlar

Spesifik

o'lchash usullari va shartlari

Sinov vositasi

Induktivlik

AL=4300±25%

(nH/N2)

1kHz/0.1V, 10Ts, 23±2 daraja

Agilent HP4284A LCR metr yoki unga tenglashtirilgan

Kompyuter quvvatini yo'qotish

Kompyuter 4 dan kichik yoki teng.0 Vt

25kHz/100mT, 100 daraja

Iwatsu SY8216 B- H analizatori yoki ekvivalenti

 

Quvvatli ferrit materiali LP3

 

Xususiyatlari

Belgi

Birlik

Vaziyat

LP3

Dastlabki o'tkazuvchanlik

μi

   

2300±25%

Nisbiy yo'qotish omili

tan/mi

×10-6

100 kHz

<4

To'yinganlik oqimining zichligi*(1194A/m)

Bs

mT

25 daraja

500

100 daraja

390

Qolganlik*

Br

mT

 

130

Majburiylik*

Hc

A/m

 

13

Quvvat yo'qolishi*

(f=100kHz,B=100mT)

Pcv

kVt/m3

25 daraja

 

80 daraja

90

100 daraja

70

Quvvat yo'qolishi*

(f=100kHz,B=200mT)

Pcv

kVt/m3

25 daraja

650

60 daraja

 

80 daraja

450

100 daraja

410

120 daraja

 

Kyuri harorati

Tc

daraja

 

215 dan katta yoki teng

Qarshilik*

ρ

Ω·m

 

5

Zichlik*

d

kg/m3×103

 

4.8

 

Eslatma: 1.Qiymatlar, agar boshqacha ko'rsatilmagan bo'lsa, xona haroratida toroidal yadro P25×P15×10 bilan olingan.

2. * Oddiy qiymat,*1Sinov holati (f=400kHz,B=50mT),*2Sinov holati (f=500kHz,B=50mT).

 

product-822-804
O'tkazuvchanlik mkiga nisbatan harorat T
product-823-804
Powerloss PCv vs. Temperature
product-825-844
Powerloss PCv va chastota f
product-824-844
Amplituda o'tkazuvchanligi mka va oqim zichligi Bm
product-822-966
Toʻyinganlik oqimining zichligi Bs va harorat T
product-822-966
To'liq zichlik B va magnit maydon H

 

 

Issiq teglar: Ferrit yadrosi uu80/65/30, Xitoy ferrit yadrosi uu80/65/30 ishlab chiqaruvchilar, etkazib beruvchilar, zavod

So'rov yuborish

(0/10)

clearall